Elektroda tangan stainless steel hidrogen rendah, sing utama
komposisi yaikukurang C-18% Cr-12% Ni-2% Mo, resistance karat titik banget
Ripple apik
kinerja welding banget, resistance retak apik
resistance porositas apik, resistance geni apik saka lapisan,
Sifat mekanik sing stabil saka logam sing digabung, tingkat pass X-Ray luwih dhuwur.
Gampang slagging
Parameter produk
KOMPONEN KIMIA:
ALLOY (wt%) | C | Mn | Si | P | S | Ni | Cr | Mo | Cu | Liyane |
ATURAN GB/T | 0.035 | 1.53 | 0.61 | 0,027 | 0.004 | 11.26 | 18.7 | 2.1 | 0.10 | - |
PROPERTI MEKANIKAL:
PROPERTI | KEKUATAN PENGHASILAN (MPa) | KEKUATAN EXTENSION (MPa) | NILAI IMPAK J/℃ | Perlakuan panas °C*h | ||||
ATURAN GB/T | 575 | 40 | - | - |
PARAMETER WELDING REKOMENDASI:
SPESIFIKASI DIAMETER (mm) | 2.0*250 | 2.6*300 | 3.2*350 | 4.0*350 | 5.0*350 | |||||
LISTRIK (Amp) | H/W | 30-55 | 50-85 | 80-120 | 100-150 | 140-180 | ||||
O/W | 20-50 | 45-80 | 70-110 | 90-135 | - |
Dhukungan pabrik
Produk kasebut cocog kanggo a
sawetara saka sudhut aplikasi
TEKNOLOGI WELDING
-
Energi Satelit Zhejiang
Tangki panyimpenan LPG 3×60.000 m³
-
49.000 ton duplex
tanker kimia stainless steel
-
JU2000E
platform pengeboran jack-up
KOMPONEN KIMIA:
ALLOY (wt%) | C | Mn | Si | P | S | Ni | Cr | Mo | Cu | Liyane |
ATURAN GB/T | 0.035 | 1.53 | 0.61 | 0,027 | 0.004 | 11.26 | 18.7 | 2.1 | 0.10 | - |
PROPERTI MEKANIKAL:
PROPERTI | KEKUATAN PENGHASILAN (MPa) | KEKUATAN EXTENSION (MPa) | NILAI IMPAK J/℃ | Perlakuan panas °C*h | ||||
ATURAN GB/T | 575 | 40 | - | - |
PARAMETER WELDING REKOMENDASI:
SPESIFIKASI DIAMETER (mm) | 2.0*250 | 2.6*300 | 3.2*350 | 4.0*350 | 5.0*350 | |||||
LISTRIK (Amp) | H/W | 30-55 | 50-85 | 80-120 | 100-150 | 140-180 | ||||
O/W | 20-50 | 45-80 | 70-110 | 90-135 | - |