Baja paduan rendah Kawat inti fluks E91T1-B3C Data pengelasan
KOMPONEN KIMIA:
ALLOY (wt%) | C | Mn | Si | Cr | Ni | Mo | P | S |
ATURAN GB/T | 0.05-0.12 | 1.25 | 0.80 | 2.0-2.5 | - | 0.90-1.20 | 0.03 | 0.03 |
ATURAN AWS | 0.05-0.12 | 1.25 | 0.80 | 2.0-2.5 | - | 0.90-1.20 | 0.03 | 0.03 |
NILAI CONTOH | 0,055 | 0.63 | 0.32 | 2.2 | 0.02 | 1 | 0.01 | 0.005 |
PROPERTI MEKANIKAL:
PROPERTI | KEKUATAN PENGHASILAN (MPa) | KEKUATAN EXTENSION (MPa) | NILAI IMPAK J/℃ | ELONGASI(%) | Perlakuan panas°Cxh | |||||
ATURAN GB/T | 540 | 620-760 | - | 15 | 690*1 | |||||
ATURAN AWS | 540 | 620-760 | - | 17 | 690*1 | |||||
NILAI CONTOH | 650 | 730 | 90/suhu normal | 20 | 690*1 |
PARAMETER WELDING REKOMENDASI:
SPESIFIKASI DIAMETER (mm) | 1.2 | ||||
Volt | 24-35 | ||||
Amp | 160-320 | ||||
dawa ekstensi garing (mm) | 15-20 | ||||
Aliran gas (l/min) | 15-25 |
Busur iku alus lan stabil, kurang cipratan, mbentuk ayu.
Aman slag apik, kurang soot.
Kanthi kinerja proses welding banget.
-
Jiangsu Donghua Energy 80.000 m3 tangki panyimpenan propana
-
Proyek LNG-2 Arktik
-
materi welding kanggo silencer
KOMPONEN KIMIA:
ALLOY (wt%) | C | Mn | Si | Cr | Ni | Mo | P | S |
ATURAN GB/T | 0.05-0.12 | 1.25 | 0.80 | 2.0-2.5 | - | 0.90-1.20 | 0.03 | 0.03 |
ATURAN AWS | 0.05-0.12 | 1.25 | 0.80 | 2.0-2.5 | - | 0.90-1.20 | 0.03 | 0.03 |
NILAI CONTOH | 0,055 | 0.63 | 0.32 | 2.2 | 0.02 | 1 | 0.01 | 0.005 |
PROPERTI MEKANIKAL:
PROPERTI | KEKUATAN PENGHASILAN (MPa) | KEKUATAN EXTENSION (MPa) | NILAI IMPAK J/℃ | ELONGASI(%) | Perlakuan panas°Cxh | |||||
ATURAN GB/T | 540 | 620-760 | - | 15 | 690*1 | |||||
ATURAN AWS | 540 | 620-760 | - | 17 | 690*1 | |||||
NILAI CONTOH | 650 | 730 | 90/suhu normal | 20 | 690*1 |
PARAMETER WELDING REKOMENDASI:
SPESIFIKASI DIAMETER (mm) | 1.2 | ||||
Volt | 24-35 | ||||
Amp | 160-320 | ||||
dawa ekstensi garing (mm) | 15-20 | ||||
Aliran gas (l/min) | 15-25 |